[STEEL FABRICATION]

Bend Allowance and Flat Pattern Development for Pressed Plate

How the neutral axis, inside radius and K-factor combine into a bend allowance, so the blank you cut actually finishes at the size on the drawing.

6 MIN READ3 SECTIONSIncludes diagram

Introduction

When plate or sheet is bent, the outside face stretches and the inside face compresses. Somewhere between them a layer keeps its original length — the neutral axis — and that layer, not the outside dimension, defines the developed length of the blank.

Bend allowance quantifies the arc length along that neutral layer. Without it, every folded part is short by roughly one plate thickness per bend, and the error compounds on multi-bend work.

bdcentroidI = Σ(bd³/12 + Ad²) about the centroid
I-section notation used for area and second moment of area

The three inputs

Three values control the result: the inside bend radius R, the material thickness t, and the K-factor, which locates the neutral axis as a fraction of thickness measured from the inside face.

For cold-formed sheet with R roughly equal to t, K is commonly taken between 0.33 and 0.45. For air bending where the radius is larger relative to thickness, K moves toward 0.5. For hot-formed plate with generous radii, the neutral axis sits close to mid-thickness.

Bend allowance and the flat length

The bend allowance is the arc length at the neutral layer: BA = θ × (R + K·t), with θ in radians. For a 90° bend, θ = π/2.

From outside dimensions, the flat length is the sum of the outside legs, minus the two setback distances, plus the bend allowance. Setback for a 90° bend is R + t measured from the outside corner. Working from tangent points instead of outside dimensions avoids the setback step entirely and is less error-prone.

  • One bend: flat = leg₁ + leg₂ − 2(R + t) + BA (outside dimensions, 90°).
  • Several bends: sum every straight length between tangent points, then add each bend allowance.
  • Confirm the K-factor against a test bend in the actual material before cutting a full run.

Why the workshop value differs from the spreadsheet

Press brake tooling, material tensile strength and grain direction all shift the real neutral axis. A development calculated with K = 0.44 can be a millimetre out over a long leg — acceptable on a bracket, not on a launder section that must fit another.

The practical fix is to bend a test piece, measure the finished outside dimensions, and back-calculate an effective K for that tool and material. Use that value for the production run.

[F]Technical formulas

Bend allowance

BA = θ × (R + K × t)

θ in radians; for 90° use π/2 = 1.5708.

Flat length (90°, outside dims)

L = a + b − 2(R + t) + BA

a and b measured to the outside corner.

Outside setback

OSSB = (R + t) × tan(θ/2)

For 90° this reduces to R + t.

[V]Explanation of variables

SymbolMeaningUnit
θBend angleradians
RInside bend radiusmm
tMaterial thicknessmm
KNeutral axis location factor–
BABend allowance (neutral axis arc length)mm

[E]Worked example

90° bend, 2 mm sheet, 3 mm inside radius

  1. 01Outside dimensions 100 mm and 60 mm to the corner; t = 2 mm, R = 3 mm, take K = 0.44.
  2. 02BA = 1.5708 × (3 + 0.44 × 2) = 1.5708 × 3.88 = 6.10 mm.
  3. 03Setback = R + t = 5 mm each side, so deduct 10 mm.
  4. 04Flat length = 100 + 60 − 10 + 6.10 = 156.1 mm.

Result

The blank is 156 mm, not 160 mm. Cutting to 160 mm would leave the finished part 4 mm oversized across the legs.

[A]Practical applications

  • Developing flat blanks for flashings, gutters and ductwork.
  • Preparing cutting lists for press-brake work.
  • Checking a supplier’s flat pattern before nesting.
  • Estimating material for multi-bend sections where waste compounds.

[!]Common mistakes

  • Using the outside dimensions as the developed length with no deduction.
  • Applying a K-factor from another material or another tool set.
  • Mixing degrees and radians in the bend allowance formula.
  • Ignoring grain direction, which changes the achievable radius and springback.

[S]References and sources

  • AS/NZS 5131 – Structural steelwork: fabrication and erectionFabrication tolerances that govern how close a formed part must be.
  • AS/NZS 1594 – Hot-rolled steel flat productsThickness and flatness tolerances for the starting plate.

Standards are cited by designation and title only — no clause text is reproduced. Purchase current editions from Standards Australia, and confirm the edition that applies to your project.

FABRICATION AND PROJECTS

Turning the take-off into a fabrication package

Mass, surface area and cutting figures become the material list a fabricator prices from. These resources cover fabrication capability and where the projects are.