Introduction
Distortion is shrinkage that could not go anywhere else. Every weld shrinks as it cools, and the structure resists that movement unevenly, so the assembly bows, cups or twists.
Correction after the fact is expensive and always risks the material. Prevention costs a change in sequence and a few jigs.
Prevention that works
Balance the weld sequence around the neutral axis so shrinkage on one side is opposed by shrinkage on the other. Backstep welding spreads the heat along a long seam, and skip welding breaks a continuous run into balanced segments.
Jigs and strongbacks hold the geometry while the weld cools. They are only effective if they are stiff enough and if they stay in place until the joint is cool, not until the arc stops.
- Weld from the centre outwards on a long seam.
- Keep the number of passes to the minimum the procedure allows.
- Use the lowest heat input that still gives fusion.
- Allow the assembly to cool in the jig rather than releasing it hot.
Controlled correction
Flame straightening works by heating a small area so that it expands against the surrounding cold metal, then contracts on cooling and pulls the member back. It is effective on mild steel and requires a temperature limit and a record.
Quenched and tempered and thermomechanically rolled steels have a maximum straightening temperature that must not be exceeded, and some grades must not be flame straightened at all without the mill recommendation. Peening is not a substitute for a proper sequence.
[F]Technical formulas
Heat input
HI = (V x A x 60) / (1000 x v)
Keep within the procedure while correcting.
Number of passes
n = weld area / pass area
Fewer passes means less total shrinkage.
Shrinkage allowance for a butt weld
allowance = shrinkage per pass x number of passes
Take the value from the procedure or the shop records.
[V]Explanation of variables
| Symbol | Meaning | Unit |
|---|---|---|
| V | Voltage | V |
| A | Current | A |
| v | Travel speed | mm/min |
| n | Number of passes | - |
[E]Worked example
An 8 mm fillet weld with 8 mm2 per pass
- 01Weld cross-section for an 8 mm fillet is about 32 mm2.
- 02At 8 mm2 per pass that is four passes.
- 03Each pass adds shrinkage, so the sequence and direction of those four passes decide the final shape.
Result
Four passes can be laid to balance each other, or to pull the member one way — the choice is made before the first arc.
[A]Practical applications
- Planning the sequence for a long stiffened plate.
- Investigating a fabricated beam that arrived bowed.
- Writing a correction procedure for a rejected item.
- Deciding whether a distortion issue is a welding or a jigging problem.
[!]Common mistakes
- Releasing a hot assembly from the jig.
- Flame straightening a quenched and tempered steel without a temperature limit.
- Using peening to hide a distortion that sequence would have prevented.
- Correcting a member that has already been drilled and marked.
[S]References and sources
- AS/NZS 1554.1 – Structural steel welding: welded steel structuresDistortion control and straightening limits for structural steelwork.
- AS/NZS 5131 – Structural steelwork: fabrication and erectionAcceptance tolerances after correction.
Standards are cited by designation and title only — no clause text is reproduced. Purchase current editions from Standards Australia, and confirm the edition that applies to your project.